WDET | WDMW
A recommended cutting conditions | PROGRAMMING DATA | A
Condições de corte recomendadas | Condiciones de corte recomendables Dados para programação | Datos para la programación
| ISO | PSM | Material | HB (Brinell) | Wear Resis | Vc (m tance | /min) | Toughness | Feed fz | (mm/t) |
| PH7910 | PH7920 | PH7930 | PH7740 | WDMW 12… | WDET 12… | ||||
| 1 | Unalloyed Steel | 125-220 | 160-280 | 150-230 | 140-220 | 100-180 | 0,30-1,50 | 0,30-1,30 | |
| P | 2 | Low-Alloyed Steel | 220-280 | 150-230 | 140-220 | 130-180 | 90-170 | 0,30-1,50 | 0,30-1,30 |
| 3 | High-Alloyed Steel | 280-380 | 140-190 | 130-180 | 100-170 | 80-140 | 0,30-1,30 | 0,30-1,00 | |
| 4 | SS - Ferritic/Martensitic | 200-330 | - | - | 130-220 | 100-180 | - | 0,30-1,30 | |
| M | 5 | SS - Austenitic | 200-330 | - | - | 120-180 | 90-150 | - | 0,30-1,30 |
| 6 | SS - Austenitic-ferritic(Duplex) | 230-260 | - | - | 70-140 | 70-120 | - | 0,30-1,00 | |
| 7 | Malleable Cast Iron | 130-230 | 160-350 | 150-310 | - | 120-240 | 0,30-1,50 | - | |
| K | 8 | GreyCast Iron | 180-245 | 150-300 | 140-260 | - | 100-200 | 0,30-1,50 | - |
| 9 | Nodular Cast iron | 160-250 | 120-260 | 100-220 | - | 80-150 | 0,30-1,40 | - | |
| S | 11 | Heat Resistant Super Alloys | 200-320 | - | - | 35-65 | 25-45 | - | 0,30-1,00 |
Rp x b ae
(Note 1) Cutting conditions ae/Dc=70%. (Note 2) It’s possible to occur vibrations in certain cases. Please reduce depth of cut and / or reduce cutting conditions in following cases: - When using long shank; - When using long tool overhang with arbor type; - When application has poor clamping rigidity or when using a low rigidity machine. (Note 3) PH5… and PHS… can be used wet or dry. PH7… use only air. (Note 4) It’s possible to occur vibrations in certain cases. Please reduce depth of cut and / or reduce cutting conditions in following cases: - When using long shank; - When using long tool overhang with arbor type; - When application has poor clamping rigidity or when using a low rigidity machine.
Descida em rampa e interpolação helicoidal | Bajada en rampa e interpolación circular DH di Lr Ramping Helical Interpolation
When using WDET insert, please remove the washer and the washer screw, otherwise it will break the insert.
Blind hole
| CHIP-BREAKER selection guide | | Dc | Flat bottom | ||
| Guia para aplicações do quebra-aparas | Guía para aplicación del rompevirutas | Ødi = ØDH - ØDc |
HB Chip-Breaker Application Ramping Helical Interpolation
| ØDc | Max Ramp aº | Ramping Max ap | Min Lr | ØDHmin | Helical Interpolation ØDHmax | Max Pitch/Rev. |
| 52 | 0,8 | 1,5 | 107,4 | 89,6 - | - 102,0 | 1 2 |
| 66 | 0,4 | 1,5 | 214,9 | 117,6 - | - 130,0 | 1 1 |
| 80 | 0,3 | 1,5 | 286,5 | 145,6 - | - 158,0 | 1 1 |
ISO PSM Material
| M | 5 | SS - Austenitic | 200-330 | WDET 12... | - |
| 7 | Malleable Cast Iron | 130-230 | WDMW 12... | - | |
| Note: During helical interpolation do not exceed max Pitch. | |||||
| K | 8 | Grey Cast Iron | 180-245 | WDMW 12... | - |
| 9 | Nodular Cast iron | 160-250 | WDMW 12... | - | |
| S | 11 | Heat Resistant Super Alloys | 200-320 | WDET 12... | - |