A End mill – UM/HPC/VSM series

Starting values for cutting speed vc[m/min]
p5501R384 5502R384 5602R38414GM (-R) 14GM (-R) 14GM (-R)5501 5502 5602R38414GM R38414GM R38414GM(-R) long (-R) long (-R) longseries series series
BrinellgrouSlotmillingShoulder millingSlotmillingShoulder milling
Material groupComposition / structure / heat treatmenthardnessningØ [mm]ap maxØ [mm]ae maxØ [mm]ap maxØ [mm]ae max
HBMachi0 < x < 30,3x D0 < x < 30.15 x D0 < x < 30,3x D0 < x < 30.15 x D
3 ≤ x < 120,7 x D3 ≤ x < 200,3 x D3 ≤ x < 120,7 x D3 ≤ x < 200,3 x D
12 ≤ x ≤ 201,5 x D12 ≤ x ≤ 201,5 x D
KMG405KMG405
ae/ Dae/ D
1/11/21/10f-group1/11/21/10f-group
approx. 0,15 % Cannealed125125030038091902252859
approx. 0,45 % Cannealed190224028536591852152759
Unalloyed steelapprox. 0,45 % Ctempered250317521027091351602009
approx. 0,75 % Cannealed270415018023091151351759
approx. 0,75 % Ctempered300514016521091051251609
Pannealed180619022528591451702159
tempered275715018023091151351759
Low-alloyed steeltempered300814016521091051251609
tempered350913016020091001201509
High-alloyed steel and high-alloyedannealed2001017521027091351602009
tool steelhardened and tempered3251113516020591051201559
ferritic/martensiticannealed200128010012596575959
M Stainless steelmartensitictempered24013708511095565809
austeniticquench hardened1801485105130965801009
austenitic-ferritic23015708511095565809
liti/fiti1801618522028091401652109
Grey cast ironpercerrc
perlitic (martensitic)2601715018023091151351759
ferritic1601822527034591752052609
K Cast iron with spheroidal graphiteperlitic2501917521027091351602009
Malleable cast ironferritic1302025030038091902252859
perlitic2302120024030591551802309
cannot be hardened6022
Aluminium wrought alloyshardenablehardened10023
≤ 12 % Si, cannot be hardened7524
Cast aluminium alloys≤ 12 % Si, hardenablehardened9025
N> 12 % Si, cannot be hardened13026
machining steel, PB> 1%11027
Copper and copper alloys (bronze/brass)CuZn, CuSnZn9028
CuSn, Pb-free copper, electrolytic copper10029
Fbd llannealed20030
e-ase aoyshardened28031
Heat-resistant alloysannealed25032
SNi or Co basshardened35033
cast32034
pure titaniumR40035
Titanium alloysα and β alloyshardenedm Rm105036
dd lhardened and tempered55 HRC371151401759
Harene steehardened and temered60 HRC38
H Hard cast ironp cast400391351652059
Hardened cast ironhardened and tempered55 HRC40
Thermoplasts Thermosetting plastics41 42
X Non-metallic materialsPlastic, glass-fibre reinforced GF ii RP i43
Plastic, carbon fibre reinforced Ci FRP44
Graphite Wood45 46

Note: The given cutting values are guide values, which were determined under ideal conditions.