| oup | SU Series | Starting | values fo | r cutting s SU-Drill | peed v | c[m/min] S | U Step Dr | ill | |||||
| Brinell | g gr | 3-5xD | 8xD | 3xD | |||||||||
| Material group | Composition / struc | ure / heat treatment | hardness HB | hinin | KDG 303 | KDG 303 | KDG 303 | ||||||
| Mac | Coolant | ||||||||||||
| Int. | Ext. | f-group | Int. | Ext. f | -grou | p Int. | Ext. | f-group | |||||
| approx. 0,15 % C | annealed | 125 | 1 | 150 | 135 | 8 | 135 | 125 | 7 | 150 | 135 | 8 | |
| approx. 0,45 % C | annealed | 190 | 2 | 130 | 120 | 8 | 120 | 110 | 7 | 130 | 120 | 8 | |
| Unalloyed steel | approx. 0,45 % C | tempered | 250 | 3 | 120 | 110 | 6 | 110 | 100 | 5 | 120 | 110 | 6 |
| approx. 0,75 % C | annealed | 270 | 4 | 110 | 100 | 6 | 100 | 90 | 5 | 110 | 100 | 6 | |
| approx. 0,75 % C | tempered | 300 | 5 | 100 | 90 | 6 | 90 | 85 | 5 | 100 | 90 | 6 | |
| P | annealed | 180 | 6 | 130 | 120 | 8 | 120 | 110 | 7 | 130 | 120 | 8 | |
| Llld tl | tempered | 275 | 7 | 110 | 100 | 6 | 100 | 90 | 5 | 110 | 100 | 6 | |
| ow-aoye see | tempered | 300 | 8 | 100 | 90 | 6 | 90 | 85 | 5 | 100 | 90 | 6 | |
| tempered | 350 | 9 | 90 | 85 | 6 | 85 | 80 | 5 | 90 | 85 | 6 | ||
| High-alloyed steel and high- | annealed | 200 | 10 | 120 | 110 | 8 | 110 | 100 | 7 | 120 | 110 | 8 | |
| alloyed tool steel | hardened and tempered | 325 | 11 | 100 | 90 | 6 | 90 | 85 | 5 | 100 | 90 | 6 | |
| ferritic/martensitic | annealed | 200 | 12 | 80 | 75 | 5 | 75 | 70 | 5 | 80 | 75 | 5 | |
| M Stainless steel | martensitic | tempered | 240 | 13 | 55 | 50 | 5 | 50 | 45 | 5 | 55 | 50 | 5 |
| austenitic | quench hardened | 180 | 14 | 60 | 55 | 5 | 55 | 50 | 5 | 60 | 55 | 5 | |
| austenitic-ferritic | 230 | 15 | 50 | 45 | 5 | 45 | 45 | 5 | 50 | 45 | 5 | ||
| perlitic/ferritic | 180 | 16 | 135 | 125 | 8 | 125 | 115 | 7 | 135 | 125 | 8 | ||
| Grey cast iron | |||||||||||||
| perlitic (martensitic) | 260 | 17 | 110 | 100 | 8 | 100 | 90 | 7 | 110 | 100 | 8 | ||
| Ciihhidl | ferritic | 160 | 18 | 120 | 110 | 8 | 110 | 100 | 7 | 120 | 110 | 8 | |
| K ast ron wt speroa graphite | perlitic | 250 | 19 | 80 | 75 | 8 | 75 | 70 | 7 | 80 | 75 | 8 | |
| Malleable cast iron | ferritic | 130 | 20 | 130 | 120 | 8 | 120 | 110 | 7 | 130 | 120 | 8 | |
| perlitic | 230 | 21 | 80 | 75 | 8 | 75 | 70 | 7 | 80 | 75 | 8 | ||
| cannot be hardened | 60 | 22 | |||||||||||
| Aluminium wrought alloys | |||||||||||||
| hardenable | hardened | 100 | 23 | ||||||||||
| ≤ 12 % Si, cannot be hardene | d | 75 | 24 | ||||||||||
| Cast aluminium alloys | ≤ 12 % Si, hardenable | hardened | 90 | 25 | |||||||||
| N | > 12 % Si, cannot be hardene | d | 130 | 26 | |||||||||
| machining steel, PB> 1% | 110 | 27 | |||||||||||
| Copper and copper alloys (bronze/brass) | CuZn, CuSnZn | 90 | 28 | ||||||||||
| CuSn, Pb-free copper, electro | lytic copper | 100 | 29 | ||||||||||
| annealed | 200 | 30 | |||||||||||
| Fe-based alloys | |||||||||||||
| hardened | 280 | 31 | |||||||||||
| Heat-resistant alloys | annealed | 250 | 32 | ||||||||||
| S | Ni or Co bass | hardened | 350 | 33 | |||||||||
| cast | 320 | 34 | |||||||||||
| pure titanium | Rm400 | 35 | |||||||||||
| Titanium alloys | α and β alloys | hardened | Rm1050 | 36 | |||||||||
| hardened and tempered | 55 HRC | 37 | |||||||||||
| Hardened steel | hardened and tempered | 60 HRC | 38 | ||||||||||
| H Hard cast iron | cast | 400 | 39 | ||||||||||
| Hardened cast iron | hardened and tempered | 55 HRC | 40 | ||||||||||
| Thermoplasts | 41 | ||||||||||||
| Thermosetting plastics | 42 | ||||||||||||
| X Non-metallic materials | Plastic, glass-fibre reinforced | i GFRP | 43 | ||||||||||
| Plastic, carbon fibre reinforce | idCFRP | 44 | |||||||||||
| Graphite Wood | 45 46 |
Note: The given cutting values are guide values, which were determined under ideal conditions. The values have to be adapted in individual cases. With hole depths of 5xD adjust the cutting data accordingly to the application. f-group = feed rate recommendations on page C126. For examples of material for cutting tool groups view page D22.