| up | Thread | S former | tarting va | lues for cutting spee Thread tap | d vc[m/mi | n] Thread milling | ||||
| Material group | Composition / struc | ture / heat treatment | Brinell hardness | ing gro | 4122A 4222A | 4122M 4222M | 4201C | 4201A 4202C | 4202A | 4111 |
| HB | chin | YK40F | YK40F | YK40F | YK40F YK40F | YK40F | KTG4015 | |||
| Ma | Coolant | |||||||||
| External | External | External | External External | External | External f-group | |||||
| approx. 0,15 % C | annealed | 125 | 1 | 20 | 100 1 | |||||
| approx. 0,45 % C | annealed | 190 | 2 | 20 | 90 1 | |||||
| Unalloyed steel | approx. 0,45 % C | tempered | 250 | 3 | 20 | 80 1 | ||||
| approx. 0,75 % C | annealed | 270 | 4 | 20 | 70 1 | |||||
| approx. 0,75 % C | tempered | 300 | 5 | 20 | 70 1 | |||||
| P | annealed | 180 | 6 | 20 | 90 1 | |||||
| Low-alloyed steel | tempered | 275 | 7 | 20 | 70 1 | |||||
| tempered | 300 | 8 | 20 | 60 1 | ||||||
| tempered | 350 | 9 | 20 | 55 1 | ||||||
| High-alloyed steel and high- | annealed | 200 | 10 | 20 | 80 1 | |||||
| alloyed tool steel | hardened and tempered | 325 | 11 | 20 | 50 1 | |||||
| ferritic/martensitic | annealed | 200 | 12 | 20 | ||||||
| M Stil tl | martensitic | tempered | 240 | 13 | 20 | |||||
| aness see | austenitic | quench hardened | 180 | 14 | 20 | |||||
| austenitic-ferritic | 230 | 15 | 20 | |||||||
| perlitic/ferritic | 180 | 16 | 20 | 20 | 80 1 | |||||
| Grey cast iron | perlitic (martensitic) | 260 | 17 | 20 | 20 | 60 1 | ||||
| Cast iron with spheroidal | ferritic | 160 | 18 | 15 | 15 | 80 1 | ||||
| K graphite | perlitic | 250 | 19 | 15 | 15 | 60 1 | ||||
| ferritic | 130 | 20 | 20 | 20 | 60 1 | |||||
| Malleable cast iron | perlitic | 230 | 21 | 20 | 20 | 80 1 | ||||
| Aluminium wrought alloys | cannot be hardened | 60 | 22 | 180 1 | ||||||
| hardenable | hardened | 100 | 23 | 150 1 | ||||||
| ≤ 12 % Si, cannot be hardene | d | 75 | 24 | 30 | 30 | 30 | 30 | 150 1 | ||
| N Cast aluminium alloys | ≤ 12 % Si, hardenable | hardened | 90 | 25 | 25 | 25 | 25 | 25 | 150 1 | |
| > 12 % Si, cannot be hardene | d | 130 | 26 | 150 1 | ||||||
| machining steel, PB> 1% | 110 | 27 | 150 1 | |||||||
| Copper and copper alloys (bronze/brass) | CuZn, CuSnZn | 90 | 28 | 150 1 | ||||||
| CuSn, Pb-free copper, electro | lytic copper | 100 | 29 | 150 1 | ||||||
| F-bd ll | annealed | 200 | 30 | |||||||
| ease aoys | hardened | 280 | 31 | |||||||
| Heat-resistant alloys | annealed | 250 | 32 | |||||||
| S | Ni or Co bass | hardened | 350 | 33 | ||||||
| cast | 320 | 34 | ||||||||
| Titanium alloys | pure titanium | Rm400 | 35 | |||||||
| α and β alloys | hardened | Rm1050 | 36 | |||||||
| hardened and tempered | 55 HRC | 37 | ||||||||
| Hardened steel | hardened and tempered | 60 HRC | 38 | |||||||
| H Hard cast iron | cast | 400 | 39 | |||||||
| Hardened cast iron | hardened and tempered | 55 HRC | 40 | |||||||
| Thermoplasts Thermosetting plastics | 41 42 | |||||||||
| X Non-metallic materials | Plastic, glass-fibre reinforced | i GFRP | 43 | |||||||
| Plastic, carbon fibre reinforce | idCFRP | 44 | ||||||||
| Graphite Wood | 45 46 |
Note: The given cutting values are guide values, which were determined under ideal conditions. The values have to be adapted in individual cases. With hole depths of 5xD adjust the cutting data accordingly to the application. f-group = feed rate recommendations on page C164. For examples of material for cutting tool groups view page D22.