A Grade STA NDA RD CUT TING CONDITIONS TPA/EPA/HPA B Hard- Cutting speed Feed per tooth: fz (mm/t) Insert Workpiece materials ness Grades Vc (m/min) MJ NMJ AJ HB T/E/HPA06 T/E/HPA10 T/EPA15 T/E/HPA06 T/E/HPA10 T/EPA15 T/EPA15 T/E/HPA10 Low carbon steel (SS400, S15C , etc. - 200 AH3135 100 - 220 100 - 250 100 - 250 0.05 - 0.15 0.08 - 0.2 0.08 - 0.25 0.08 - 0.15 - E275A, C15E4, etc. C Ext. Toolholder High carbon steel S45C, etc. 200 - 300 AH3135 100 - 170 100 - 200 100 - 230 0.05 - 0.12 0.08 - 0.15 0.08 - 0.2 0.08 - 0.15 - C45, etc. Alloy steel SCM440, etc. 150 - 300 AH3135 100 - 170 100 - 200 100 - 230 0.05 - 0.12 0.08 - 0.15 0.08 - 0.2 0.08 - 0.15 - 42CrMo4, etc. Tool steel D 30 - 40 Int. Toolholder SKD61, etc. AH3135 100 - 120 100 -150 100 - 180 0.05 - 0.12 0.08 - 0.15 0.08 - 0.2 0.08 - 0.15 - X40CrMoV5-1, etc HRC Stainless steel SUS304, etc. - AH3135 80 - 150 80 - 200 90 - 200 0.05 - 0.15 0.08 - 0.2 0.08 - 0.2 0.08 - 0.15 - X5CrNi18-9, etc. Grey cast iron AH120 100 - 200 100 - 250 140 - 250 0.05 - 0.15 0.08 - 0.2 0.08 - 0.25 0.08 - 0.15 - FC250, etc. 150 - 250 E T1215 150 - 250 150 - 300 200 - 300 0.05 - 0.12 0.08 - 0.15 0.08 - 0.18 - - Threading 250, etc. Ductile cast iron AH120 80 - 150 80 - 200 110 - 200 0.05 - 0.15 0.08 - 0.2 0.08 - 0.25 0.08 - 0.15 - FCD450, etc. 150 - 250 450-10S, etc. T1215 100 - 200 130 - 250 150 - 250 0.05 - 0.12 0.08 - 0.15 0.08 - 0.18 - - Aluminium Si < 13% - KS05F - 300 - 1000 - - - - - 0.08 - 0.22 F Grooving Aluminium - KS05F - 100 - 200 - - - - - 0.08 - 0.22 Si ≥ 13% Titanium alloys - AH120 20 - 50 20 - 60 20 - 60 0.05 - 0.1 0.08 - 0.15 0.08 - 0.18 0.08 - 0.15 - Ti-6Al-4V, etc. Milling cutter Miniature tool G Heat-resistant alloys - AH120 20 - 35 20 - 40 20 - 40 0.03 - 0.08 0.05 - 0.13 0.07 - 0.15 0.07 - 0.15 - Inconel 718, etc. · When you use the NMJ chipbreaker, please set up the feed less than 0.15 mm/t. · Cutting conditions maybe limited depending on machine power, workpiece · Remove excessive chip accumulation with an air blast. rigidity, and spindle output. When the cutting width, depth, or overhang · For the operation with depth of cut which varies (ex.casting skin) and length is large, set Vc and fz to the lower recommended values and check machining of workpiece materials with interrupted surface, the feed per tooth the machine power and vibration. H (fz) should be set to the lower recommended value shown in the above table. TLA (Roughing type) I Cutting speed Feed per tooth: fz (mm/t) Hardness Vc (m/min) Endmill ISO Workpiece materials Grades MJ NMJ AJ HB TLA10 TLA15 TLA10 TLA15 TLA15 TLA10 Low carbon steel SS400, S15C, etc. - 200 AH3135 100 - 250 100 - 250 0.08 - 0.18 0.08 - 0.22 0.08 - 0.15 - E275A, C15E4, etc. J High carbon steel Drilling tool S45C, etc. 200 - 300 AH3135 100 - 200 100 - 270 0.08 - 0.14 0.08 - 0.18 0.08 - 0.15 - C45, etc. Alloy steel 30 - 40 SCM440, etc. AH3135 100 - 150 100 - 180 0.08 - 0.14 0.08 - 0.18 0.08 - 0.15 - 42CrMo4, etc. HRC Stainless steel User's Guide Tooling System K SUS304, etc. - AH3135 80 - 200 90 - 200 0.08 - 0.15 0.08 - 0.18 0.08 - 0.15 - X5CrNi18-9, etc. Grey cast iron AH120 100 - 250 140 - 250 0.08 - 0.18 0.08 - 0.25 0.08 - 0.15 - FC250, etc. 150 - 250 250, etc. T1215 150 - 250 150 - 250 0.08 - 0.15 0.08 - 0.18 - - Ductile cast iron AH120 80 - 200 110 - 200 0.08 - 0.18 0.08 - 0.25 0.08 - 0.15 - FCD450, etc. 150 - 250 450-10S, etc. T1215 150 - 250 150 - 250 0.08 - 0.15 0.08 - 0.18 - - Aluminium Si < 13% Aluminium Si ≥ 13% - - KS05F KS05F 300 - 1000 100 - 200 - - - - - - - - 0.08 - 0.22 0.08 - 0.22 L M Titanium alloys - AH120 20 - 60 20 - 60 0.08 - 0.15 0.08 - 0.18 0.08 - 0.15 - Ti-6Al-4V, etc. Index Heat-resistant alloys - AH120 20 - 40 20 - 40 0.05 - 0.13 0.07 - 0.15 0.07 - 0.15 - Inconel 718, etc. · When using NMJ chipbreaker, please set up the feed not to exceed 0.15 mm/t. Tungaloy H133