Tensile strength [N/mm2] AK2010 AK2110 AK2310 AK2320 AM2030 AM2035 AM2110 AM2130 AM5015 AM5020 AM5025 Recommended Cutting Data Turning – Carbide coated Cutting speed Vc [m/min] ISO Material ca. 0,15% C 350 - 220 - 380 220 - 380 200 - 340 170 - 220 180 - 230 - - 220 - 320 180 - 230 180 - 230 Unalloyed steel and cast steel ca. 0,45% C 650 - 190 - 330 190 - 330 180 - 290 160 - 180 170 - 190 - - 180 - 290 170 - 190 170 - 190 ca. 0,75% C 1000 - 160 - 280 160 - 280 150 - 240 120 - 140 130 - 150 - - 150 - 250 130 - 150 130 - 150 600 - 180 - 300 180 - 300 170 - 260 160 - 180 170 - 190 - - 180 - 280 170 - 190 170 - 190 P Low alloyed steel and cast steel 900 - 160 - 260 160 - 260 150 - 240 80 - 140 90 - 150 - - 170 - 250 90 - 150 90 - 1501200-120 - 220120 - 220120 - 22060 - 12070 - 130--150 - 22070 - 13070 - 130 High alloyed steel, high alloyed annealed 700 - 140 - 220 140 - 220 140 - 200 110 - 190 120 - 200 - - 80 - 160 120 - 200 120 - 200 tool steel and cast steel hardened and tempered 1100 - 70 - 130 70 - 130 70 - 120 40 - 90 50 - 100 - - 40 - 130 50 - 100 50 - 100 ferritic / martensitic, annealed 700 - 140 - 220 140 - 220 140 - 220 130 - 170 140 - 180 - - 60 - 180 140 - 180 140 - 180 Stainless steel and cast steel martensitic, hardened and tempered 1000 - 70 - 130 70 - 130 70 - 110 100 - 150 110 - 140 - - 40 - 140 110 - 140 110 - 140 M Stainless steel and cast steel austenitic and austenitic/ferriticchilled 450 - 600 - - - - 100 - 180 100 - 180 120 - 200 100 - 140 80 - 160 120 - 200 120 - 200600 - 900----70 - 14070 - 14070 - 18070 - 14040 - 13090 - 16090 - 160 pearlitic, ferritic 500 - 700 150 - 210 250 - 380 250 - 380 250 - 340 - - - - 180 - 300 - 120 - 160 Cast iron pearlitic, martensitic 700 - 850 220 - 350 190 - 300 190 - 300 190 - 250 - - - - 160 - 280 - 90 - 130 800 - 1100 - - - - - - 120 - 240 - - K Cast iron with nodular graphite ferritic 550 220 - 380 220 - 300 220 - 300 200 - 260 - - - - 140 - 230 - 120 - 160 pearlitic 800 200 - 350 150 - 230 150 - 230 150 - 200 - - - - 120 - 170 - 120 - 180 ferritic 450 200 - 400 200 - 300 200 - 300 200 - 260 - - - - 150 - 210 - 140 - 220 Malleable cast iron pearlitic 750 180 - 320 170 - 230 170 - 230 170 - 200 - - - - 150 - 210 - 110 - 160 not heat treatable 200 - - - - - - - - - - - Aluminum alloys, long chipping heat treatable, heat treated 350 - - - - - - - - - - - ≤ 12% Si, hardened 250 - - - - - - - - - - - Casted aluminum alloys ≤ 12% Si, heat treatable, hardened 300 - - - - - - - - - - - ≤ 12% Si, not heat treatable 450 - - - - - - - - - - - N Copper and copper alloys Lead alloys, Pb > 1%Brass, bronze 400 - - - - - - - - 200 - 500 - -300--------200 - 500-- (brass / bronze) Aluminum bronze 500 - - - - - - - - 160 - 450 - - Copper and electrolyte copper 200 - - - - - - - - 100 - 320 - - Duroplastics - - - - - - - - 160 - 600 - - Non-ferrous materials Reinforced plastics - - - - - - - - 100 - 300 - - Hard rubber - - - - - - - - - - - Fe-alloyed annealed 700 - - - - 20 - 40 20 - 40 - - 20 - 60 - 20 - 50 Fe-alloyed hardened 950 - - - - 15 - 35 15 - 35 - - 20 - 60 - 20 - 50 High temperature resistant alloys Ni- oder Co- based annealed 800 - - - - 8 - 25 8 - 25 - - 15 - 50 - 15 - 40 S Ni- oder Co- based casting 1100 - - - - 4 - 15 4 - 15 - - 15 - 40 - 10 - 25 i Ni- oder Co- based hardened 1200 - - - - 4 - 15 4 - 15 - - 15 - 40 - 20 - 35Titanium alloys, high strengthPure titanium500 - 700----80 - 13080 - 130--90 - 180-80 - 140 Alpha- and beta-alloys, hardened 700 - 1000 - - - - 15 - 35 15 - 35 - - 40 - 80 - 25 - 45 hardened and tempered 1000 - 1350 - - - - - - - - 30 - 50 - - Hardened steel H Hard cast iron hardened and tempered 1350 - 1700 - - - - - - - - 10 - 25 - -casting1350---------40 - 70-- Hardened cast iron hardened and tempered 1900 - - - - - - - - 10 - 25 - - The datas cutting speeds given are approximate values. More grades on the It is necessary to adjust them to the individual machining operation. following pages. 450 ARNO®-Werkzeuge | Drehen | Turning | Точение