| Материал | Инструментальны стали SKD, 1.2344, 1.2379,1.23 | е и штамповые SKH, NAK 11, P20 (45HRC) | Закаленн SKD, 1.2344, (45~55 | ые стали SKT 1.2379 HRC) | Закаленн SKD, 1.2344, (55~65 | ые стали SKH 1.2379 HRC) |
| Вид обработки | ap 0.1D ae 0.3D D ae ap | ap 0.05D (max ae 0.1D ae ap | 0.5mm) D | ap 0.03D (ma ae 0.05D ae ap | x 0.3mm) D | |
| Диаметр | n (мин-1) | Vf (мм/мин) | n (мин-1) | Vf (мм/мин) | n (мин-1) | Vf (мм/мин) |
| 1 | 32,000 | 1,600 | 25,000 | 1,300 | 22,000 | 1,100 |
| 2 | 28,000 | 1,700 | 22,000 | 1,400 | 20,000 | 1,200 |
| 3 | 24,000 | 1,800 | 21,000 | 1,500 | 18,000 | 1,300 |
| 4 | 20,000 | 2,000 | 18,000 | 1,600 | 14,000 | 1,400 |
| 6 | 16,000 | 2,200 | 13,000 | 1,800 | 10,000 | 1,500 |
| 8 | 12,000 | 2,300 | 10,000 | 2,000 | 8,000 | 1,500 |
| 10 | 10,000 | 2,200 | 8,000 | 1,800 | 6,000 | 1,400 |
| 12 | 8,000 | 2,000 | 6,500 | 1,700 | 5,000 | 1,200 |
| 16 | 6,000 | 1,800 | 5,000 | 1,500 | 4,000 | 1,000 |
| 20 | 5,000 | 1,500 | 4,000 | 1,200 | 3,000 | 800 |
| 25 | 4,000 | 1,200 | 4,000 | 1,000 | 2,000 | 600 |
Примечание: Режимы резания должны быть скорректированы в зависимости от жесткости системы СПИД станка и условий обработки.